We have measured the critical current
(Ic) of a high
current density Nb3Sn
strand subjected to spatial periodic bending, periodic contact stress and uniaxial strain.
The strand is destined for the cable-in-conduit conductors (CICC) of the European dipole
(EDIPO) 12.5 T superconducting magnet test facility. The spatial periodic bending was
applied on the strand, using the bending wavelengths from 5 to 10 mm with a peak
bending strain of 1.5%, a periodic contact stress with a periodicity of 4.7 mm and
a stress level exceeding 250 MPa. For the uniaxial strain characterization, the
voltage–current characteristics were measured with an applied axial strain from
−0.9% to
+0.3%, with a magnetic field from 6 to 14 T, temperature from 4.2 to 10 K and currents up to
almost 900 A. In addition the axial stiffness was determined by a tensile axial stress–strain
test. The characterization of the strand is essential for understanding the behaviour of the
strand under mainly axial thermal stress variation during cool down and transverse
electromagnetic forces during charging, which is essential for the design of the CICC for the
dipole magnet.
The strand appears to be fully reversible in the compressive regime during the axial
strain testing, while in the tensile regime, the behaviour is already irreversibly
degraded when reaching the maximum in the critical current versus strain
characteristic. The degradation is accentuated by an immediate decrease of the
n
value by a factor of 2. The parameters for the improved deviatoric strain description are derived from
the Ic
data, giving the accuracy of the scaling with a standard deviation of 4 A, which is by far
within the expected deviation for the large scale strand production of such a high
Jc strand.
The Ic
versus the applied bending strain follows the low resistivity limit, indicative of full
interfilament current transfer, while a strong decrease is observed at a peak bending strain of
∼0.5%. For the periodic contact stress it appears that beyond 60 MPa, the
Ic becomes noticeably
irreversible. The n
value, being a better indicator for the irreversible behaviour than the
Ic, seems to indicate a somewhat lower level of the transverse stress irreversibility. Since the
strand appears to be quite sensitive to the tensile strain, for the EDIPO CICC design,
the tensile intrinsic axial strain in the filamentary region should stay well below
zero (only compressive) and the contact stress sufficiently below 50 MPa. These
requirements are feasible, in particular for a CICC design with steel conduit which would
provide sufficient thermal compression, a sufficiently low void fraction and a cabling
pattern that limits the peak bending strain during transverse load to about 0.3%.