The preparation of porous copper or copper-zinc surfaces by electrochemical formation of binary Equation or symbol description not availableCu–Zn alloys on Cu substrate and subsequent electrochemical etching of the zinc was investigated in a zinc chloride-1-ethyl-3-methylimidazolium chloride ionic liquid at Equation or symbol description not available120°C. Cyclic voltammetry and X-ray diffraction measurements suggested that phase transformation from γ- to β′-Equation or symbol description not availableCu–Zn alloy occurred during constant potential dealloying. Essentially all the Zn content in the Equation or symbol description not availableCu–Zn could be removed from the alloy with dealloying at a sufficiently positive potential. Dealloyed materials exhibited well-developed bicontinuous porous structure. The dependence of the surface morphology of the porous Cu film on several experimental parameters, including deposition current and charge, and anodizing potential and temperature, were examined.