Lithium-rich transition-metal oxides lose oxygen during the first removal of lithium. In this study, the kinetics of the oxygen-loss process of the lithium-rich oxide, Equation or symbol description not availableLi[Li1/9Ni1/3Mn5/9]O2, of varying particle sizes was studied. The electrochemical data were analyzed, and oxygen diffusion constants of Equation or symbol description not available3×10−13 and Equation or symbol description not available2×10−12cm2s−1 were determined for the oxygen-loss process at 30 and Equation or symbol description not available55°C, respectively. This is about 1000 times smaller than typical lithium diffusion constants in layered oxides. The Equation or symbol description not availableLi[Li1/9Ni1/3Mn5/9]O2 material with a Equation or symbol description not available3μm particle size was cycled without capacity loss at a specific capacity of Equation or symbol description not available240mAhg−1 at Equation or symbol description not available55°C.