Platinum and platinum oxide films were deposited by remote plasma atomic layer deposition (ALD) from the combination of (methylcyclopentadienyl)trimethylplatinum Equation or symbol description not available(MeCpPtMe3) precursor and Equation or symbol description not availableO2 plasma. A short Equation or symbol description not availableO2 plasma exposure (0.5 s) resulted in low resistivity Equation or symbol description not available(15μΩcm), high density Equation or symbol description not available(21g/cm3), cubic Pt films, whereas a longer Equation or symbol description not availableO2 plasma exposure (5 s) resulted in semiconductive Equation or symbol description not availablePtO2 films. In situ spectroscopic ellipsometry studies revealed no significant nucleation delay, different from the thermal ALD process with Equation or symbol description not availableO2 gas which was used as a benchmark. A broad temperature window Equation or symbol description not available(100–300°C) for remote plasma ALD of Pt and Equation or symbol description not availablePtO2 was demonstrated.