The effect of part per billion (ppb) levels of Equation or symbol description not availableSO2 on the atmospheric corrosion on Al (99.999%) was investigated in the laboratory at 22°C. Exposure time was 20 and 672 h. The effect of Equation or symbol description not availableSO2 concentration (46-1300 ppb), relative humidity (70-99% RH), and the amount of NaCl applied prior to exposure Equation or symbol description not available(0-250μg∕cm2) was studied. In addition, the effect of Equation or symbol description not availableO3 and Equation or symbol description not availableNO2 on the Equation or symbol description not availableSO2 deposition rate was addressed. The samples were investigated by gravimetry, grazing incidence X-ray powder diffraction, ion chromatography, optical microscopy, and environmental scanning electron microscopy equipped with energy-dispersive X-ray fluorescence. Equation or symbol description not availableSO2 accelerates the atmospheric corrosion of Al, forming corrosion product “islands” containing aluminum hydroxy sulfate. Combining NaCl and Equation or symbol description not availableSO2 has a synergistic effect on the average corrosion rate. In contrast, the chloride-induced pitting of aluminum is significantly reduced by Equation or symbol description not availableSO2. The corrosivity of Equation or symbol description not availableSO2 is attributed to the acidification of the surface electrolyte that destabilizes the alumina passive film. The suppression of pitting corrosion by Equation or symbol description not availableSO2 is attributed to the formation of aluminum hydroxy sulfates that are less soluble than the corresponding chlorides and slows down pit propagation. At relative humidities above 70% RH, there is a measurable steady-state deposition of Equation or symbol description not availableSO2 that corresponds to the rate of formation of sulfate. The Equation or symbol description not availableSO2 deposition rate is not limited by the oxidation of (IV)-valent sulfur on the surface. Equation or symbol description not availableSO2 deposition is enhanced by sodium chloride because the corrosion reactions in the NaCl(aq) electrolyte result in high pH in the cathodic regions and the formation of aluminum hydroxide. Ozone in the ppb range has only transient effects on the Equation or symbol description not availableSO2 deposition rate, whereas ppb levels of Equation or symbol description not availableNO2 had no effect at all.