The effect of UV-ozone pretreatment of AlGaN/GaN high electron mobility transistor (HEMT) surfaces prior to Equation or symbol description not availableSiNx passivation is reported. Without pretreatment, breakdown voltages dropped from 60 V (the test maximum) to ∼5 V, and interdevice isolation current increased from Equation or symbol description not available10−9 to Equation or symbol description not available10−6 A following plasma-enhanced chemical vapor deposition Equation or symbol description not availableSiNx passivation. With pretreatment, breakdown voltages dropped from 60 to ∼58 V, and interdevice isolation current increased from Equation or symbol description not available10−9 to Equation or symbol description not available∼10−8 A following Equation or symbol description not availableSiNx passivation. Transmission electron microscopy and X-ray photoelectron spectroscopy measurements showed the formation of a 15-25 Å thick GaO layer as a result of the UV-Ozone treatment. HEMT device results showed that UV-ozone pretreatment does not degrade the ability of the Equation or symbol description not availableSiNx to provide effective surface passivation and reduce current collapse. © 2004 The Electrochemical Society. All rights reserved.