A Equation or symbol description not availableCaAl2O4:Eu2+,Nd3+,Sr2+ phosphor, with white light under irradiation and a yellow-green long afterglow, was prepared by the solid-state method. The emission spectra, afterglow spectra, and afterglow decay curve of the samples have been measured. It is found that the emission spectra under the irradiation of Equation or symbol description not available400nm are comprised of the blue-light emission Equation or symbol description not available(442nm) and the yellow-green-light emission Equation or symbol description not available(538nm), and the chromaticity coordinates were calculated to be Equation or symbol description not availablex=0.289, Equation or symbol description not availabley=0.341. After the irradiation source was removed, the blue emission decreased rapidly so that the white-light photoluminescence changed to the yellow-green afterglow and its persistent time was measured to be over Equation or symbol description not available4h.