Titanium was severely attacked when immersed in a molten alkali chloride bath in the presence of air. The most severe corrosion of this metal was observed in molten Equation or symbol description not availableNaCl‐NaF mixtures; samples disintegrated completely at temperatures of 850°C in less than 3 hr. Progressively less corrosion occurred in Equation or symbol description not availableKCl, Equation or symbol description not availableNaCl, and Equation or symbol description not availableLiCl melts. In many cases, salt fumes were more corrosive than the molten salt itself, evidently because of the better access of oxygen to the titanium surface. The corrosion rate fluctuated greatly from test to test but was very low in experiments performed in vacuum.

The chief corrosion products were a dispersion of metallic titanium in the molten salt (“pyrosols”), mixed with some titanium oxides. The mixture was dark gray, and colored the solid salt bluish‐black. White to yellowish oxides appeared in small amounts on the surface of the salt bath and consisted mainly of Equation or symbol description not availableTiO2.