The photoresist strip rate at the edge and center of an array of silicon wafers is calculated for an oxygen plasma. The etch rate at the edge is essentially independent of wafer diameter and spacing, whereas the etch rate at the center increases linearly with increasing wafer spacing and is inversely proportional to the square of wafer diameter. Thus, a plasma stripping or etching system has a processing rate which can be specified in silicon area per unit time. The degree of inhomogeneity between edge and center also depends on the probability of reaction when a reactive specie hits the photoresist. Experimental measurements confirm the predicted functional dependence, except with an oxygen plasma the strip rate at the center of the wafer varies inversely as the cube of the wafer diameter rather than as the square. The implication is that two atomic oxygen atoms react simultaneously with the photoresist, perhaps as Equation or symbol description not availableCH2+2O→CO+H2O, or more probably as Equation or symbol description not availableO+O+wall→O2+wall.