Abstract
To investigate whether unsaturated
vapor can have effects in hot corrosion, experiments have been conducted wherein specimens cut from
turbine blades were sprayed with
, and then exposed in a tube furnace at 1625°F under an air stream containing
(1/20 the
saturation pressure at 1625°F) with inspection and sulfate recoating every 24 hr. Several chloride effects were evident within 100–200 hr under this test regime. These included: (i) increasing the
vaporization rate; (ii) causing formation of a spalling
surface oxide; (iii) removing Cr by the formation of volatile complexes which apparently contain S and Na as well as Cr and Cl; (iv) interacting with Ti at the coatingblade interface; and (v) accelerating sulfidation‐oxidation attack upon the
coating. This latter attack occurs when both blade metal and coating are exposed simultaneously to the sulfate, as at a cut edge. It is confined to the
layer, and consists of a sulfidation front and oxidation front which traverse the coating successively, effectively stripping the coating from the supposedly less resistant blade alloy. Sodium chloride increases the kinetics of attack and appears to promote the formation of
over
as the predominate sulfide phase. A search for chloride was made by energy‐dispersive x‐ray analysis in the SEM, but despite the obvious
influences, no trace of chloride was found except possibly in the Ti interaction. The individual
effects are discussed in relation to earlier research results and as they may pertain to shipboard hot corrosion.