Metallic tungsten film has been obtained by potentiostatic electrolysis in Equation or symbol description not availableZnCl2-NaCl-KCl (0.60:0.20:0.20, in mole fraction) melt containing Equation or symbol description not availableWCl4 at Equation or symbol description not available250°C. The deposit obtained after the electrolysis at Equation or symbol description not available0.02V vs. Equation or symbol description not availableZn(II)∕Zn for Equation or symbol description not available3h was ca. Equation or symbol description not available0.5μm thick and the surface was not smooth. On the other hand, addition of Equation or symbol description not available4mol% of KF to the melt gave a smooth metal deposit ca. Equation or symbol description not available0.5μm thick in the same condition as above.