The Equation or symbol description not availableSrBi2Ta2O9 (SBT) films were successfully deposited on Equation or symbol description not availablePt/Ti/SiO2/Si substrates by liquid delivery metallorganic chemical vapor deposition (MOCVD) with a single cocktail of Equation or symbol description not availableSr[Ta(OEt)5(dmae)]2/(OEt:OC2H5,dmae:C4H10NO) and Equation or symbol description not availableBi(C6H5)3. The Bi/Ta mol ratio increases and Sr/Ta decreases with increasing deposition temperature at a precursor mol ratio of 0.5. At the deposition temperature of 400°C and in range of 0.5 to 1 of the precursor mol ratio, Sr/Ta and Bi/Ta ratio in SBT are close to 0.4 and 1.1, which matches the required Sr/Ta and Bi/Ta ratio in SBT thin films. The step coverage of SBT films obtained at aspect ratio of 1 is about 90% and is suitable for high density memory device application. The remanent polarization Equation or symbol description not available(2Pr) and coercive field Equation or symbol description not available(Ec) of Equation or symbol description not availableSr0.8Bi2.2Ta2.0O9 thin films annealed at 750°C were 13 μC/cm2 and 52 kV/cm at an applied voltage of 5 V. The SBT films annealed at 750°C showed practically no polarization fatigue up to Equation or symbol description not available1010 switching cycles. © 2001 The Electrochemical Society. All rights reserved.