We fabricated FePt films on thermal-oxidized Si substrate by rapid thermal annealing (RTA), and obtained (001)-oriented FePt/L10 small grains. By varying the total thickness of as-deposited Pt/Fe layers, we obtain isolated FePt/L10 crystalline grains after RTA. The smallest average grain size was only 7 nm in diameter. These as-deposited Pt/Fe layers were uniform and have a smooth surface; however after RTA, cohesion occurred and FePt/L10 small crystalline particles appeared. After annealing, the FePt grains are embedded in the SiO layer. The films showed high Hc and high remanence ratio in the direction perpendicular to the film plane. The FePt Curie temperature is appoximately 400°C.